How to store batteries (BU20)
Batteries are perishable products that start deteriorating right from
the moment they leave the factory. There are simple preventive measures
that battery users can apply to slow the aging process. This paper
provides guidelines to reduce age-related capacity losses and how
to prime new and stored batteries.
The recommended storage temperature for most batteries is 15°C
(59°F). While lead-acid batteries must always be kept at full
charge, nickel and lithium-based chemistries should be stored at 40%
state-of-charge (SoC). This level minimizes age-related capacity loss,
yet keeps the battery in operating condition even with some self-discharge.
While the open terminal voltage of nickel-based batteries cannot be
used to determine the SoC accurately, voltage fuel gauging works well
for lithium-ion cells. However, differences in the electrochemistry
of the electrodes and electrolyte between manufacturers vary the voltage
profile slightly. A SoC of 50% reads about 3.8V; 40% is 3.75V. Store
lithium-ion at an open terminal voltage of 3.75-3.80V. Allow the battery
to rest 90 minutes after charge before taking the voltage reading.
Figure 1 illustrates the recoverable capacity at various storage temperatures
and charge levels over one year.
Figure 1: Non-recoverable capacity loss on lithium-ion and
nickel-based batteries after storage. High charge levels and elevated
temperatures hasten the capacity loss.
Among
the lithium-ion family, cobalt has a slight advantage over manganese (spinel)
in terms of storage at elevated temperatures. nickel-based batteries are also
affected by elevated temperature but to a lesser degree than lithium-ion.
Lithium-ion powers most of today's laptop computers. The battery compartment
on many laptops rises to about 45°C (113°F) during operation. The combination
of high charge level and elevated ambient temperature presents an unfavorable
condition for the battery. This explains the short lifespan of many laptop batteries.
Nickel-metal-hydride
can be stored for about three years. The capacity drop that occurs during storage
is permanent and cannot be reversed. Cool temperatures and a partial charge slows
aging. Nickel-cadmium stores reasonably well. Field test reveled that NiCd batteries
stored for five years still performed well after priming cycles. Alkaline and
lithium batteries (primary) can be stored for up to 10 years. The capacity loss
is minimal. The sealed lead-acid battery can be stored for up to two
years. A periodic topping charge, also referred to as 'refresh charge', is required
to prevent the open cell voltage from dropping below 2.10V. (Some lead-acid batteries
may allow lower voltage levels.) Insufficient charge induces sulfation, an oxidation
layer on the negative plate that inhibits the current flow on charge and discharge.
Topping charge and/or cycling may restore some of the capacity losses in the early
stages. Priming
new batteries
Manufacturers recommend to trickle charge a nickel-based battery for 24 hours
when new and after long storage. This service brings all cells to equal charge
level and redistributes the electrolyte to remedy dry spots on the separator brought
on by gravitation of the electrolyte. It is advisable to verify the capacity with
a battery analyzer before use. This is especially important in critical applications.
Cycling (priming) is recommended to regain lost capacity after a nickel-based
battery has been stored for 6 months or longer. A slow charge followed by one
or several discharge/charge cycles will do this. The recovery rate is governed
by the condition under which the battery was stored. The longer and warmer the
storage temperature, the more cycles will be required. The Prime program of the
Cadex battery analyzers automatically applies the number of cycles needed to regain
full capacity. Nickel-based batteries are not always fully formed when
leaving the factory. Applying several charge/ discharge cycles through normal
use or with a battery analyzer completes the forming. The number of cycles needed
to attain full capacity differs between cell manufacturers. Quality cells perform
to specification after 5-7 cycles. Those lacking formation may need 50 or more
cycles to reach acceptable capacity levels. What is the difference between
priming and forming? For the user, both symptoms manifest themselves as insufficient
capacity. The difference may be explained in that forming needs to be done only
once when the battery is new, while priming must be repeated after each prolonged
storage. Lithium-ion batteries deliver full power after the initial
charge. Manufacturers of lithium-ion cells insist that no priming is required.
However, priming is beneficial as an initial start and to verify battery performance.
Excessive cycling should be avoided because of wear-down effect. The
internal protection circuit of lithium-based batteries is known to cause some
problems after a long storage. If the battery is left discharged after use, the
self-discharge will further drain the pack and eventually drip the protection
circuit at about 2.5 volts per cell. At this point, the charger will no longer
recognize the battery and the pack appears dead. Advanced battery analyzers (Cadex)
feature the Boost program that activates the protection circuit to enable
a recharge. If the cell voltage has fallen below 1.5V/cell and has remained in
that state for a few days, a recharge should be avoided for safety reasons.
To reduce the self-discharge on newly manufactured batteries, advanced lithium-ion
packs feature a sleep mode that keeps the protection circuit off until activated
by a brief charge. Once engaged, the battery remains operational and the advantage
of the sleep mode no longer applies. Lead-acid batteries should be primed
by applying a full charge, followed by a discharge and recharge. Verifying the
capacity through a discharge is important, especially if the battery is engaged
in critical applications such as powering medical devices. Priming is also recommended
after storing a battery for six months and longer. Battery analyzers provide the
priming service automatically.
It is believed that a partial or full discharge applied once every six months
or so enhances the performance of lead-acid batteries. Avoid too many full discharges,
as this would wear down the battery unnecessarily. While
capacity loss during a battery's life cannot be eliminated, simple guidelines
minimize the effect: - Keep batteries in a cool and dry storage area.
Refrigeration is recommended but freezers should be avoided. When refrigerated,
the battery should be placed in a plastic bag to protect against condensation
- Do not fully charge lithium and nickel-based batteries before storage. Keep
them partially charged and apply a full charge before use. Store lithium-ion at
about 40% state-of-charge (3.75-3.80V/cell open terminal). Lead-acid batteries
must be stored fully charged.
- Do not store lithium-ion fully depleted.
If empty, charge for about 30 minutes before storage. Self-discharge on a depleted
battery may cause the protection circuit to trip, preventing a recharge.
-
Do not stockpile lithium-ion batteries; avoid buying dated stock, even if offered
at a reduced price. Observe the manufacturing date, if available.
- Never
leave a nickel-based battery sitting on a charger for more than a few days. Prolonged
trickle charge causes crystalline formation (memory).
- Always store a
lead acid battery in full-charge condition. Observe the open terminal voltage
and recharge the battery every 6 months or as recommended by the manufacturer.
_________________________
Created: May 2003, Last edited: March 2004
About
the Author Isidor Buchmann is the founder and CEO of Cadex Electronics
Inc., in Vancouver BC. Mr. Buchmann has a background in radio communications
and has studied the behavior of rechargeable batteries in practical, everyday
applications for two decades. Award winning author of many articles and books
on batteries, Mr. Buchmann has delivered technical papers around the world.
Cadex Electronics is a manufacturer of advanced battery chargers, battery analyzers
and PC software. For product information please visit www.cadex.com.
Click
here for a printer-friendly version
©
Copyright 2003 - 2005 Isidor Buchmann
| |