Skip to main content

BU-804c: Acid Stratification and Surface Charge

Explore simple guidelines to prolong lead acid batteries by proper use
 

Acid Stratification

The electrolyte of a stratified battery concentrates at the bottom, starving the upper half of the cell. Acid stratification occurs if the battery dwells at low charge (below 80 percent), never receives a full charge and has shallow discharges. Driving a car for short distances with power-robbing accessories engaged contributes to acid stratification because the alternator cannot always apply a saturated charge. Large luxury cars are especially prone to acid stratification. This is not a battery defect per se but is application related. Figure 1 illustrates a normal battery in which the acid is equally distributed from top to bottom.

Normal battery

Figure 1: Normal battery [1]

The acid is equally distributed from the top to the bottom of the battery, providing good overall performance.

Figure 2 shows a stratified battery in which the acid concentration is light on top and heavy on the bottom. The light acid on top limits plate activation, promotes corrosion and reduces the performance, while the high acid concentration on the bottom makes the battery appear more charged than it is and artificially raises the open circuit voltage. The unequal charge across the plates reduces CCA (cold cranking amps), and starting the engine is sluggish.

Stratified battery

Figure 2: Stratified battery [1]

The acid concentration is light on top and heavy on the bottom. This raises the open circuit voltage and the battery appears fully charged. Excessive acid concentration induces sulfation on the lower half of the plates.

Allowing the battery to rest for a few days, doing a shaking motion or tipping the battery on its side helps correct the problem. Applying an equalizing charge by raising the voltage of a 12-volt battery to 16 volts for 1–2 hours also helps by mixing the electrolyte through electrolysis. Avoid extending the topping charge beyond its recommended time. Topping charge is applied to maintain full charge and to prevent sulfation on lead acid batteries.

Acid stratification cannot always be avoided. During cold winter months, starter batteries of most passenger cars dwell at a 75 percent charge level. Knowing that motor idling and driving in gridlocked traffic does not sufficiently charge the battery; charge the battery occasionally with an external charger. If this is not practical, switch to an AGM battery. AGM does not suffer from acid stratification and is less sensitive to sulfation if undercharged than the flooded version. AGM is a bit more expensive than the flooded version but the battery should last longer.
 

Surface Charge

Lead acid batteries are sluggish and cannot convert lead sulfate to lead and lead dioxide quickly during charge. This delayed action causes most of the charge activities to occur on the plate surfaces, resulting in an elevated state-of-charge (SoC) on the outside.

A battery with surface charge has a slightly elevated voltage and gives a false voltage-based SoC reading. To normalize the condition, switch on electrical loads to remove about 1 percent of the battery’s capacity or allow the battery to rest for a few hours. Turning on the headlights for a few minutes will do this. Surface charge is not a battery defect but a reversible condition.

Simple Guidelines for Extending Battery Life

  • Allow a fully saturated charge of 14–16 hours. Charge in a well-ventilated area.
     

  • Always keep lead acid charged. Avoid storage below 2.07V/cell or at a specific gravity level below 1.190.
     

  • Avoid deep discharges. The deeper the discharge, the shorter the battery life will be. A brief charge on a 1–2 hour break during heavy use prolongs battery life.
     

  • Never allow the electrolyte to drop below the tops of the plates. Exposed plates sulfate and become inactive. When low, add only enough water to cover the exposed plates before charging. Always fill to the correct level after charge.
     

  • Never add acid. This would raise the specific gravity too high and cause excessive corrosion.
     

  • Use distilled or de-ionized water. Tap water may be usable in some regions.
     

  • When new, a deep-cycle battery may have a capacity of 70 percent or less. Formatting as part of field use will gradually increase performance. Apply a gentle load for the first five cycles to allow a new battery to format.
     

  • New batteries with low capacity many not perform as well as those that begin life with a high capacity. Low performers are known to have a short life. A capacity check as part of acceptance is advisable.
     

  • A start-stop battery typically has 25 percent more lead than a standard starter battery to attain a high cycle count. This is reflected in the corresponding price premium.